CREATION GROUP · COLD FORMING SOLUTIONS中国 · 中文站

COLD FORMING MATERIALS

C17 E2 C 冷镦用钢丝 (CHQ)

MATERIALSENGINEERINGCREATION GROUP
CREATION GROUP / ZH
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
产品中心 / C17 E2 C 冷镦用钢丝 (CHQ)

C17 E2 C 冷镦用钢丝 (CHQ)

C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
C17 E2 C 冷镦用钢丝 (CHQ)
left
right
直径: 0.40-46mm
拉伸强度: 参考技术信息

上海创造集团是中国专注于冷轧优质钢丝的标杆企业,整个管理团队拥有20年的行业经验。我们与多家汽车行业一级供应商建立了良好的关系,所有钢丝均来自品牌钢厂。所有订单均100%可追溯。

img1 img1 img1

Specification

+AR 或 +PE

+AC 或 +AC+PE

+AR+C

+AR+C+AC

+AR+C+AC+LC

+AC+C

img1 img1 img1

Specification

- : 连续且平滑

- : 无接缝、重叠、坑坑、划痕和拉拔划痕

- : 不应有锈迹

img1 img1 img1
img1 img1 img1

Specification

- : 汽车产业

- : 建筑业

- : 机械行业

- : 其他行业

img1 img1 img1
Case Study

Products & Service

Related Products

C17 E2 C 冷镦用钢丝 (CHQ)

Prepainted Aluminium Coil

C17 E2 C 冷镦用钢丝 (CHQ)

Prepainted Aluminium Coil

C17 E2 C 冷镦用钢丝 (CHQ)

Prepainted Aluminium Coil

1.交货条款组合

表B.1 -交货时热处理条件、产品形式和适用要求的组合

Heat-treatment condition at deliverySymbolProducts form aApplicable requirements in cases where the steel concerned has been ordered with reference to the steel names indicated in
Wire rodBarWireTablesB.2,B.3,B.4 or B.5TablesB.2,B.3,B.4,B.5,B.6 or B,7Optional
As hot-rolled or peeled+AR or +PEXXXChemical composition as specified in Table B.2Mechanical  properties as specified in TablesB.3,B.4 and B.5Chemical compositior as specified in Table B.2Mechanical  properties as specified inTablesB,3,B.4 and B.5Values for hardenability according to Tables B.6 and B.7Supplementa- ry or special requirements as specified in Annex Eh
Cold drawn+AR+C-XX
Cold drawn + spheroidized+AR+C+AC-XX
Cold drawn + spheroidized+skin passed+AR+C+AC +LC-XX
Spheroidized or spheroidized+peeled+AC or +AC +PEXXX
Spheroidized+cold drawn+AC+C XX
Treated to ferrite- pearlite structure and hardness range+FP-X-
OthersOther delivery conditions may be agreed at the time of ordering
a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order.

2.化学成分

表B.2 -表面硬化用钢的化学成分(适用于铸造分析)

Steel name b% mass fraction a
  C  Si c  Mn  P    S  Cr  Ni  Mo  B  Cu
Non-alloy steel grades
C10E2C0,08 to 0,120,300,30 to 0,600,0250,025  0,25
C15E2C0,13 to 0,170,300,30 to 0,600,0250,025 0,25
C17E2C0,15 to 0,190,300,60 to 0,900,0250,025 0,25
C20E2C0,18 to 0,220,300,30 to 0,600,0250,025 0,25
Alloy steel grades
18MnB40,16 to 0,200,300,90 to 1,200,0250,025 0,0008 to 0,0050,25
22MnR40,20 to 0,240,300,90 to 1,200,0250,025——0,0008 to 0,0050,25
17Cr30,12 to 0,200,300,60 to 0,900,0250,0250,70 to 1,250,25
17CrS30,12 to 0,200,300,60 to 0,900,0250,020 to 0,0400,70 to 1,250,25
20Cr40,17 to 0,230,300,60 to 0,900,0250,0250,90 to 1,200,25
20CrS40,17 to 0,230,300,60 to 0,900,0250,020 to 0,0400,90 to 1,200,25
16MnCr50,14 to 0,190,301,00 to 1,300,0250,0250,80 to 1,10 0,25
16MnCrS50,14 to 0,190,301,00 to 1,300,0250,020 to 0,0400,80 to 1,10 0,25
16MnCrB50,14 to 0,190,301,00 to 1,300,0250,0250,80 to 1,100,0008 to 0,0050,25
20MnCrS50,17 to 0,220,301,10 to 1,400,0250,020 to 0,0401,00 to 1,300,25
12CrMo40,10 to 0,150,300,60 to 0,900,0250,0250,90 to 1,200,15 to 0,250,25
18CrMo40,15 to 0,210,300,60 to 0,900,0250,0250,90 to 1,200,15 to 0,250,25
18CrMoS40,15 to 0,210,300,60 to 0,900,0250,020 to 0,0400,90 to 1,200,15 to 0,250,25
20MoCr40,17 to 0,230,300,70 to 1,000,0250,0250,30 to 0,60 0,40 to 0,50 0,25
20MoCrS40,17 to 0,230,300,70 to 1,000,0250,020 to 0,0400,30 to 0,600,40 to 0,500,25
Elements not quoted in this table should not be intentionally added to the steel without the agreement of the purchaser,except those intended for finishing the heat.All reasonable precautions shall be taken in order to prevent the addition of such elements from scrap or other materials used in the production process,which can affect the hardenability, mechanical properties and applicability To improve the performance of cold heading,it is possible to add Al:0,020 %to 0,050 % a Maximum values unless otherwise indicated. b In the case of steels with hardenability requirements (see Tables B.6 and B.Z),minor deviations from the specified limits are permitted (with the exception of sulfur and phosphorus),provided that they do not exceed 0,01 %for carbon and the values indicated in Table 2 for the other elements. c A lower silicon content or a specific silicon range may be agreed at the time of ordering

3.力学性能

表B.3 -非合金钢牌号的机械性能

    Steel nameDiameterDelivery condition
+AR or+PE+AC or+AC+PE+AR+C+AR+C+AC+AR+C+AC+LC+AC+C
above mmup to mmRm max. MPaZa min. %Rm max MPaZ min. %Rm max. MPaZ min. %Rm max MPaZ min. %Rm max. MPaZ min. %Rm max. MPaZ min. %
    C10E2C25 3906743065
510450584006554056380674206549062
1040450584006553056380674206548062
401004505840065     —— 
    C15E2C25      4206746065  
510480584306557056410674506552062
1040480584306556056410674506551062
401004805843065  —— 
    C17E2C25———— 4406748065
510530584506563056430674706555062
1040530584506562056430674706554062
401005305845065 ——
    C20E2C25    4606750065  
510530584706564056450674906558062
1040530584706563056450674906557062
401005305847065 ————
a The values are given only for information.

4.硬化性要求

线材捆扎示例
线材捆扎示例
成品标签示例
成品标签示例
卷材的卷绕方式
卷材的卷绕方式

外包装示例

端面木板包装
端面木板包装
缠绕包装
缠绕包装
PP布袋套袋包装
PP布袋套袋包装
线架包装
线架包装
栈板包装
栈板包装

集团技术资源

fastener-wire.com ↗