上海睿雄实业集团是中国专注于冷镦优质钢丝的标杆企业。整个管理团队拥有20年的行业经验。我们与许多汽车行业的一级供应商建立了良好的关系,所有线材均来自品牌钢厂。所有订单都100% 可追踪。
COLD FORMING MATERIALS
X6NiCrTiMoVB25-15-2 冷镦用钢丝 (CHQ)
MATERIALSENGINEERINGCREATION GROUP
CREATION GROUP / ZH

X6NiCrTiMoVB25-15-2 冷镦用钢丝 (CHQ)
1.交货条件的组合
表D.1-交货时热处理条件、产品形式和适用要求的组合
| Heat-treat- ment con- dition at delivery | Symbol | Product form a | Steel a | Applicable requirements | ||||||
| Wire rod | Bar | Wire | Ferri- tic | Marten- sitic | Austenit- ic and austenit- ic- ferritic | |||||
| Solution annealed or solution annealed +peeled | +AT or AT+PE | X | X | X | — | 一 | X | Chemical compo- sition as specified inTable D.2 | Mechani- cal prop- erties as speci- fied in Tables D.3, D.4 and D.6 | Supple- mentary or special re- quirements as specified in Annex Eb |
| Solution annealed +cold drawn | +AT+C | 一 | X | X | — | — | X | |||
| Solution an- nealed +cold drawn + solution an- nealed | +AT+C +AT | X | X | X | ||||||
| Solution an- nealed +cold drawn+solu- tion annealed + skin passed | +AT+C +AT+ LC | X | X | X | ||||||
| Soft annealed or soft annealed + peeled | +A or +A+PE | X | X | X | X | X | — | |||
| Soft annealed + skin passed | +A+LC | — | X | X | X | X | — | |||
| Soft annealed + cold drawn + soft annealed | +A+C +A | X | X | X | X | |||||
| Soft annealed + cold drawn+ soft annealed + skin passed | +A+C +A+LC | — | X | X | X | X | — | |||
| Others | Other delivery conditions may be agreed at the time of enquiry and order. | |||||||||
| a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order | ||||||||||
2.化学组成
表D.2-不锈钢牌号的化学成分 (适用于铸造分析)
| Designation | % mass fraction a | ||||||||||||||||||||||
| Steel name | ISO steel number | C | Si | Mn | P | S | Cr | Ni | Mo | N | Cu | Others | |||||||||||
| Austenitic steels | |||||||||||||||||||||||
| X10CrNi18-8 | 4310-301-00-1 | 0,05 to 0,15 | 2,00 | 2,00 | 0,045 | 0,015 | 16,0 to 19,0 | 6,0 to 9,5 | 0,80 | 0,10 | 1,00 | — | |||||||||||
| X2CrNi18-9 | 4307-304- 03-1 | 0,030 | 1,00 | 2,00 | 0,045 | 0,030 | 17,5 to 19,5 | 8,0 to 10,0 | 一 | 0,10 | 1,00 | — | |||||||||||
| X6CrNiCu18-9-2 | 4567-304- 98-X | 0,08 | 1,00 | 2,00 | 0,045 | 0,030 | 17,0 to 19,0 | 8,0 to 10.5 | 0,10 | 1,00 to 3,00 | — | ||||||||||||
| X3CrNiCu18-9-4 | 4567-304-30-1 | 0,04 | 1,00 | 2,00 | 0,045 | 0,030 | 17,0 to 19,0 | 8,5 to 10,5 b | — | 0,10 | 3,00 to 4,00 | — | |||||||||||
| X3CrNiCu19-9-2 | 4560-304- 75-E | 0,035 | 1,00 | 1,50 to 2,00 | 0,045 | 0,015 | 18,0 to 19,0 | 8,0 to 9,0 | — | 0,10 | 1,50 to 2,00 | — | |||||||||||
| X5CrNi18-10 | 4301-304- 00-1 | 0,07 | 1,00 | 2,00 | 0,045 | 0,030 | 17,5 to 19,5 | 8,0 to 10,5 | — | 0,10 | 1,00 | — | |||||||||||
| X6CrNiTi18-10 | 4541-321-00-1 | 0,08 | 1,00 | 2,00 | 0,045 | 0,030 | 17,0 to 19,0 | 9,0 to 12,0 | 一 | 1,00 | Ti=5xC to 0,70 | ||||||||||||
| X2CrNi19-11 | 4306-304- 03-1 | 0,030 | 1,00 | 2,00 | 0,045 | 0,030 | 18,0 to 20,0 | 10,0 to 12,0 | — | 0,10 | 1,00 | — | |||||||||||
| X6CrNi18-12 | 4303-305- 00-I | 0,08 | 1,00 | 2,00 | 0,045 | 0,030 | 17,0 to 19,0- | 10,5 to 13,0 | 0,10 | — | —— | ||||||||||||
| X3NiCr18-16 | 4839-384- 00-1 | 0,04d | 1,00 | 2,00 | 0,045 | 0,030 | 15,0 to 17,0 | 17,0 to 19,0 | — | 一 | —— | ||||||||||||
| Austenitic steels with Mo | |||||||||||||||||||||||
| X2CrNiMo17-12-2 | 4404-316- 03-1 | 0,030 | 1,00 | 2,00 | 0,045 | 0,030 | 16,5 to 18,5 | 10,0 to 13,0 | 2,00 to 3,00 | 0,10 | 1,00 | ||||||||||||
| Elements not quoted in this table may not be intentionally added to the steel without the agreement of the purchaser except for finishing the heat.All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production that would impair mechanical properties and the suitability of the steel. Maximum values unless otherwise indicated A minimum content of8,0 %of Niis permitted,unless otherwise agreed at the time of enquiry and order. For this document,a range for Cr:16,5 to 19,0 is allowed. d For this document,C:0,08 is allowed. In order to improve the cold formability,a carbon content of max.0,04 %is recommended and may be agreed at the time of enquiry and order. | |||||||||||||||||||||||
| Designation | % mass fraction a | |||||||||||
| Steel name | ISO steel number | C | Si | Mn | P | S | Cr | Ni | Mo | N | Cu | Others |
| X5CrNiMo17-12-2 | 4401-316- 00-I | 0,07 | 1,00 | 2,00 | 0,045 | 0,030 | 16,5 to 18,5 | 10,0 to 13,0 | 2,00 to 3,00 | 0,10 | 1,00 | — |
| X6CrNiMoTi17-12-2 | 4571-316-35-1 | 0,08 | 1,00 | 2,00 | 0,045 | 0,030 | 16,5 to 18,5 | 10,5 to 13,5 | 2,00 to 2,50 | 一 | 1,00 | Ti=5xC to 0,70 |
| X2CrNiMo17-12-3 | 4432-316-03-1 | 0,030 | 1,00 | 2,00 | 0,045 | 0,015 | 16,5 to 18,5 | 10,5 to 13,0 | 2,50 to 3,00 | 0,10 | 1,00 | 一 |
| X3CrNiMo17-13-3 | 4436-316- 00-1 | 0,05 | 1,00 | 2,00 | 0,045 | 0,015 | 16,5 to 18,5 | 10,5 to 13,0 | 2,50 to 3,00 | 0,10 | — | 一 |
| X2CrNiMoN17-13-3 | 4429-316- 53-I | 0,030 | 1,00 | 2,00 | 0,045 | 0,015 | 16,5 to 18,5 | 10,5 to 13,0 | 2,50 to 3,00 | 0,12 to 0,22 | 1,00 | — |
| X3CrNiCu- Mo17-11-3-2 | 4578-316- 76-E | 0,04 | 1,00 | 2,00 | 0,045 | 0,015 | 16,5 to 17,5 | 10,0 to 11,0 | 2,00 to 2,50 | 0,10 | 3,00 to 3,50 | 一 |
| X6NiCFTj MoVB25-15-2 | 4980-662- 86-X | 0,08 | 1,00 | 2,00 | 0,040 | 0,030 | 13,5 to 16,0 | 24,0 to 27,0 | 1,00 to 1,50 | 一 | Ti:1,90 to 2,35 Al:0,35 V:0,10 to 0,50 B:0,001 to 0,010 | |
| Austenitic-ferritic steel | ||||||||||||
| X2CrNiMoN22-5-3 | 4462-318- 03-1 | 0,030 | 1,00 | 2,00 | 0,035 | 0,015 | 21,0 to 23,0 | 4,5 to 6,5 | 2,50 to 3,50 | 0,10 to 0,22 | — | — |
| Ferritic steels | ||||||||||||
| Elements not quoted in this table may not be intentionally added to the steel without the agreement of the purchaser except for finishing the heat.All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production that would impair mechanical properties and the suitability of the steel. Maximum values unless otherwise indicated. A minimum content of 8,0 %of Ni is permitted,unless otherwise agreed at the time of enquiry and order. For this document,a range for Cr:16,5 to 19,0 is allowed. d For this document,C:0,08 is allowed. In order to improve the cold formability,a carbon content of max.0,04 %is recommended and may be agreed at the time of enquiry and order. | ||||||||||||
| Designation | % mass fraction a | |||||||||||
| Steel name | ISO steel number | C | Si | Mn | P | S | Cr | Ni | Mo | N | Cu | Others |
| X6Cr17 | 4016-430- 00-1 | 0,08 | 1,00 | 1,00 | 0,040 | 0,030 | 16,0 to 18,0 | — | — | — | — | — |
| X6CrMo17-1 | 4113-434- 00-1 | 0,08 | 1,00 | 1,00 | 0,040 | 0,030 | 16,0 to 18,0 | 一 | 0,75 to 1,40 | 一 | — | 一 |
| Martensitic steel | ||||||||||||
| X12Cr13 | 4006-410- 00-1 | 0,08 to 0,15 | 1,00 | 1,50 | 0,040 | 0,030 | 11,5 to 13,5 | 0,75 | — | — | — | |
| Elements not quoted in this table may not be intentionally added to the steel without the agreement of the purchaser except for finishing the heat.All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production that would impair mechanical properties and the suitability of the steel. a Maximum values unless otherwise indicated. b A minimum content of 8,0 %of Ni is permitted,unless otherwise agreed at the time of enquiry and order c For this document,a range for Cr:16,5 to 19,0 is allowed. d For this document,C:0,08 is allowed. In order to improve the cold formability,a carbon content of max.0,04 %is recommended and may be agreed at the time of enquiry and order. | ||||||||||||
3.机械性能
表D.6-规定交货条件下马氏体不锈钢的机械性能
| Designation | Diameter | Delivery condition | |||||||||
| +A or +A+PE | +A+LC | +A+C+A | +A+C+A+LC | ||||||||
| Steel name | ISO steel number | above mm | up to mm | Rm max. MPa | Z min. % | Rm max. MPa | Z min. % | Rm max. MPa | Z min. % | Rm max. MPa | Z min. % |
| X12Cr13 | 4006-410- 00-1 | 0,8 | 2 | 740 | 58 | ||||||
| 2 | 5 | — | —— | —— | 600 | 60 | 660 | 58 | |||
| 5 | 10 | 600 | 60 | 720 | 57 | 600 | 60 | 640 | 58 | ||
| 10 | 25 | 600 | 60 | 700 | 57 | 600 | 60 | 640 | 58 | ||
| 25 | 100 | 600 | 60 | — | — | — | — | — | |||
1、 成卷
线材捆扎示例
2、 长条状
线材捆扎示例
3、 外销木箱包装
线材捆扎示例
4、 装柜照片
装柜照片
5、 产品防护细节
产品防护
5、 产品防护细节
产品防护
外包装示例
端面木板包装
缠绕包装
PP布袋套袋包装
线架包装